Hi all,
I know this is a long shot, but I was after any information from the community regarding a set of sulfide material produced by Gerald Czamankse at the USGS in the early 70's. More to the point whether they were usable, and if so is there any still kicking about for use?
Cheers
Quote from: BenjaminWade on February 18, 2015, 03:49:05 PM
I know this is a long shot, but I was after any information from the community regarding a set of sulfide material produced by Gerald Czamankse at the USGS in the early 70's. More to the point whether they were usable, and if so is there any still kicking about for use?
I remember those standards. There were some mounted up when I started at Berkeley many years ago, but there was no extra material I think. You might ask Sean Mulcahy there though.
Some of these are listed in my default standard database:
Selected Standards:
St 617 PbS (synthetic)
St 617 PbS (synthetic)
TakeOff = 40.0 KiloVolt = 15.0 Density = 7.500
From Czemanske
(assumed stoichiometric)
Elemental Composition
Average Total Oxygen: .000 Average Total Weight%: 99.990
Average Calculated Oxygen: .000 Average Atomic Number: 73.155
Average Excess Oxygen: .000 Average Atomic Weight: 119.628
ELEM: Pb S
XRAY: ma ka
ELWT: 86.590 13.400
KFAC: .8696 .1431
ZCOR: .9958 .9366
AT% : 50.001 49.999
St 620 CuFeS2 (synthetic)
St 620 CuFeS2 (synthetic)
TakeOff = 40.0 KiloVolt = 15.0 Density = 4.200
From Czemanske (Chalcopyrite)
(assumed stoichiometric)
Elemental Composition
Average Total Oxygen: .000 Average Total Weight%: 100.000
Average Calculated Oxygen: .000 Average Atomic Number: 23.544
Average Excess Oxygen: .000 Average Atomic Weight: 45.878
ELEM: Cu Fe S
XRAY: ka ka ka
ELWT: 34.620 30.430 34.950
KFAC: .3152 .3027 .3151
ZCOR: 1.0984 1.0052 1.1093
AT% : 24.994 24.998 50.007
St 624 Ag2S (synthetic)
St 624 Ag2S (synthetic)
TakeOff = 40.0 KiloVolt = 15.0 Density = 7.300
From Alpha Aesar (#89473)
99.9+%, Lot #030281
Assumed stoichiometric
Elemental Composition
Average Total Oxygen: .000 Average Total Weight%: 100.000
Average Calculated Oxygen: .000 Average Atomic Number: 42.989
Average Excess Oxygen: .000 Average Atomic Weight: 82.599
ELEM: Ag S
XRAY: la ka
ELWT: 87.060 12.940
KFAC: .8258 .1322
ZCOR: 1.0542 .9791
AT% : 66.666 33.334
St 625 AgBiS2 (synthetic)
St 625 AgBiS2 (synthetic)
TakeOff = 40.0 KiloVolt = 15.0 Density = 6.900
From Czemanske
Elemental Composition
Average Total Oxygen: .000 Average Total Weight%: 100.000
Average Calculated Oxygen: .000 Average Atomic Number: 61.529
Average Excess Oxygen: .000 Average Atomic Weight: 95.244
ELEM: Bi Ag S
XRAY: ma la ka
ELWT: 54.854 28.314 16.833
KFAC: .5382 .2201 .1749
ZCOR: 1.0191 1.2866 .9627
AT% : 25.000 25.000 50.000
St 626 As2S3 (synthetic)
St 626 As2S3 (synthetic)
TakeOff = 40.0 KiloVolt = 15.0 Density = 3.490
From Czemanske
May be AsS (orange color)
Large grains, difficult to see in reflection
Elemental Composition
Average Total Oxygen: .000 Average Total Weight%: 100.000
Average Calculated Oxygen: .000 Average Atomic Number: 26.354
Average Excess Oxygen: .000 Average Atomic Weight: 49.207
ELEM: As S
XRAY: la ka
ELWT: 60.903 39.097
KFAC: .5700 .3214
ZCOR: 1.0686 1.2164
AT% : 40.000 60.000
Great, thanks Probeman! I will email Sean and see what happens.