Hi all
I am hoping that someone can give me some advice about analysing Troilite. What I thought should be very straight forward is turning me crazy. To give you some background I have a user who is attempting to analyse some troilite (amongst other sulfides which are coming out fine), and we are continuously overestimating the Fe content getting ~64.5% Fe (Stoichiometric troilite is Fe: 63.53% S: 36.47%). We are pretty much spot on with our S measurements. Beam conditions used are 20kV/20nA with a range of beam sizes from focussed to 10um. I am assuming 20nA is OK to use, perhaps I should be reducing it? I turned on TDI's at one point and had a look at the Fe signal and it is pretty rock solid.
Initially we were getting much too low Fe contents (~61%) until I discovered that for whatever reason (Fe-S vs Fe-S2 bonding?) compared to the Fe standard/s I peaked on (Astimex marcasite, P&H Chalcopyrite) there was quite a large peak shift in Fe towards lower values in the troilite. I checked the peak position for Fe in my 3 standards and they are within a few sintheta units of each other, but quite different to that in the troilite sample (~10 units). Following this discovery at the start of every troilite analysis I was peakscanning for Fe (and S) and was hoping this would fix my low Fe problem, but has seemed to now push it too far the other way with high Fe.
As such I am getting totals of ~101-101.5% with Fe anywhere from 64.5-65% no matter which of my limited FeS standards I use (Astimex marcasite, Astimex Pentlandite, P&H Chalcopyrite). I have had a literature scour and there are obviously a number of papers that have analysed troilite via EPMA, and its interesting to note is that in a lot of them Fe is always underestimated by ~1wt% with no explanation as to why (peakshift?).
Does anyone have any experience successfully analysing troilite and ideas of what I am doing wrong here. I am suspecting a standardisation problem but cant say for sure. Does a troilite standard exist? I know of the meteorite Canyon Diablo of which the troilite is used as a Sulfur isotope standard. Not sure if they are homogeneous in Fe/S though.
Cheers
Hi Ben,
I might be remembering this incorrectly but I seem to remember that Troilite is very beam sensitive in that the electron beam can change the composition.
I would try two tactics: first try using a larger beam/lower beam current, second try the TDI correction.
I would be very interested in seeing what you find.
john
Hi John
Ok thanks. I had already tried the TDI to no real effect and the Fe counts looked pretty solid, but might try lowering the beam current to 10nA and trying an even bigger beam. Stay tuned.
Cheers
I haven't done troilite myself (only pyrrhotite) but it sounds like you should definitely use the shifted Fe peak position for the troilite. Maybe it's not only the peak shift but also the shape? Have you tried integrated intensities?
Ok great thanks Karsten, and no I haven't actually investigated the peak shape. Good idea I will try the integrated intensities.
Yes weird thing is they are also running pyrrhotite which is coming out fine...
Have you played with different matrix corrections?
Deon.
Quote from: Karsten Goemann on May 17, 2016, 09:02:37 PM
I haven't done troilite myself (only pyrrhotite) but it sounds like you should definitely use the shifted Fe peak position for the troilite. Maybe it's not only the peak shift but also the shape? Have you tried integrated intensities?
The Fe Ka peak shape is unlikely to change, but sulfur Ka, absolutely yes. You aren't using the Fe La line are you?
But if you are using the Fe Ka line, I'm not sure why a sulfur peak shape change (actually it's a peak shift from would sulfate to pyrite to pyrrhotite), would cause the Fe intensity to be too high.
I've gotten good results for troilite using synthetic pyrrhotite (Fe7S8) as a standard for Fe and S; I'm not aware of any beam sensitivity issues, nor have I ever noted any obvious shifts in Fe Ka peak position or change in shape amongst different sulfides, other minerals, or Fe metal. Keep in mind that the Fe contents of the standards you are using (marcasite, chalcopyrite, pentlandite) are all much lower than that of troilite. Note also that Fe in pentlandite is subject to fluorescence by the Ni K lines. I tried once to analyze pyrrhotite using pyrite as a standard for Fe and S (taking the small shift in S Ka peak position into account) and got very poor results (low totals), though I can't remember if one element or the other was more problematic.
the biggest problem is FeS is rarely bang-on stoichiometric. Additionally, depending on formation conditions, it can also contain appreciable oxygen.
This has some consequences for estimating the chemical activity of Fe in FeS, but I won't bore you senseless!
Hi all
Awesome, thankyou all for the comments.
Definitely using the Fe Ka line. I am a bit puzzled now then. I definitely did see a peakshift in Fe on the users troilite sample compared to my Fe standards. I haven't had time yet to properly check the peak shapes but that is the next thing I will do. I will also check S Ka.
Brian can I ask where you got your synthetic pyrrhotite from? I have attached a copy of the paper they are trying to duplicate the methods of in which the authors are attempting to very accurately measure the Fe/S ratio in troilite, from which they calculate structural information and verify by HR-TEM. You can skip down to page 719 where they have their microprobe data in which they also mention they use an in-house natural Ni-free pyrrhotite from Dalengorsk mine in Russia. I can find many mineral specimens of pyrrhotite from Dalengorsk on ebay etc but quite reticent to spend a couple of hundred dollars on a specimen that may well be useless.
They also they use 15kV for their troilite. I guess there is no real problem with that for the levels of the elements and lines they are measuring. Could be another thing to try as well.
cheers
Hi Ben,
The synthetic pyrrhotites that I use were made by R.G. Arnold (see Econ. Geol. 57:72-90) and Louis Cabri in the 1960s and 1970s. Unfortunately I don't have any loose material.
Natural terrestrial, essentially stoichiometric troilite can be obtained from some localities in Oregon and far northern California (Del Norte County), where it occurs in serpentinite in the Josephine Ophiolite.
Have you thought about trying to synthesize pyrrhotite/troilite yourself? I haven't done it, but it should be relatively easy to do by sealing Fe powder/sponge and sulfur in an evacuated silica glass tube and then heating in a muffle furnace. It ought to be possible to produce stoichiometric material by saturating the system in Fe (and so then weighing the starting materials precisely wouldn't be critical). I can send phase diagrams if you'd like.
Brian
Hi Brian
That would be great if you could send the phase diagrams through if you have them on hand. This student is heading back to China and he says they can attempt to create it in his lab back home as they have had some experience synthesising Fe sulfides pretty much exactly as you describe. If I can give him the phase diagrams that would be great. I will also see if I can chase up some hand specimens of serpentinite from those localities.
I am going to try a recalibration at 15kV with peak integration today but not holding out much hope. I also noticed that using XPP over Armstrong/Love alleviated the problem a little but don't think I am justified in forcing the data to fit that way, I still think its a standard problem. Will let you all know how it goes..
Cheers
EDIT: Hi all. I am in the process of trying the integrated intensities, and noticed that the wavescan it is doing on Fe and S is very fast. I can change the number of steps no problems in the Elements/Cations box, but not matter what count times I change for Wave/Peak scan I cant get it to slow down. Is there some way I can change the count times of the wavescan it does during the Peak integration scan?
Hi Ben,
I've attached a paper showing details of the Fe-S phase diagram. Hope this is helpful.
Brian
Excellent, thanks Brian.
Cheers
Just to reply to my own thread...
John in an earlier post I edited I was having a problem slowing the peak scanning down for integrated intensities:
Quote from: BenjaminWade on May 19, 2016, 05:32:05 PM
EDIT: Hi all. I am in the process of trying the integrated intensities, and noticed that the wavescan it is doing on Fe and S is very fast. I can change the number of steps no problems in the Elements/Cations box, but not matter what count times I change for Wave/Peak scan I cant get it to slow down. Is there some way I can change the count times of the wavescan it does during the Peak integration scan?
Can this be done or is this a fixed speed? I imagine it can be done given you can change the step sizes for the integration scan.
cheers
Quote from: BenjaminWade on May 25, 2016, 07:33:13 PM
Just to reply to my own thread...
John in an earlier post I edited I was having a problem slowing the peak scanning down for integrated intensities:
Quote from: BenjaminWade on May 19, 2016, 05:32:05 PM
EDIT: Hi all. I am in the process of trying the integrated intensities, and noticed that the wavescan it is doing on Fe and S is very fast. I can change the number of steps no problems in the Elements/Cations box, but not matter what count times I change for Wave/Peak scan I cant get it to slow down. Is there some way I can change the count times of the wavescan it does during the Peak integration scan?
Can this be done or is this a fixed speed? I imagine it can be done given you can change the step sizes for the integration scan.
cheers
Hi Ben,
I will need to look at this when I get back to Eugene.
john
Quote from: BenjaminWade on May 25, 2016, 07:33:13 PM
Just to reply to my own thread...
John in an earlier post I edited I was having a problem slowing the peak scanning down for integrated intensities:
Quote from: BenjaminWade on May 19, 2016, 05:32:05 PM
EDIT: Hi all. I am in the process of trying the integrated intensities, and noticed that the wavescan it is doing on Fe and S is very fast. I can change the number of steps no problems in the Elements/Cations box, but not matter what count times I change for Wave/Peak scan I cant get it to slow down. Is there some way I can change the count times of the wavescan it does during the Peak integration scan?
Can this be done or is this a fixed speed? I imagine it can be done given you can change the step sizes for the integration scan.
cheers
Hi Ben,
I fooled myself for a moment when looking into this, but it turns out not to be a bug. The deal is, the on-peak count time is for the *full* scan. So if you put in 10 seconds, each point will be a fraction of that time. You can put in say 120 seconds and will see it takes longer. It is true that this could have been clearer so I added some text to the count time dialog. I checked both the step/count integrated scanning and also the ROM integrated scanning. They both seem to work.
But there was a small display bug in the graph so I fixed that and also added the current count time per point to the x axis label since it varies as a function of intensity.
Download the latest PFE v. 11.51 and you should be OK.
john
Awesome, thanks again John. I was trying to alter it via wavescan timing, but didn't even think of using the on peak count time to alter it.
Just FYI we conducted the troilite analysis using what we had at the time with the fast peak scanning. It was hard with the superfast integrated intensities to notice fine moves in peak shift, but some were definitely very different and some not at all. Which is strange but its a natural troilite sample so who knows what kind of variation to expect in it. In addition there were definitely peak shifts in S Ka as we might expect. Totals ranged from too low now (by 1-2 wt%), however some were very close to what we might expect.
We are hoping to rerun his samples again soon now with the slower integrated intensities and will see what happens. He is also getting his lab back in Nanjing to send us some of their synthetic troilite which we might play around with.
Cheers
Quote from: BenjaminWade on June 05, 2016, 05:12:51 PM
Awesome, thanks again John. I was trying to alter it via wavescan timing, but didn't even think of using the on peak count time to alter it.
Just FYI we conducted the troilite analysis using what we had at the time with the fast peak scanning. It was hard with the superfast integrated intensities to notice fine moves in peak shift, but some were definitely very different and some not at all. Which is strange but its a natural troilite sample so who knows what kind of variation to expect in it. In addition there were definitely peak shifts in S Ka as we might expect. Totals ranged from too low now (by 1-2 wt%), however some were very close to what we might expect.
We are hoping to rerun his samples again soon now with the slower integrated intensities and will see what happens. He is also getting his lab back in Nanjing to send us some of their synthetic troilite which we might play around with.
Cheers
Although one can do excellent quant on sulfides/sulfates using different peaked positions for each phase, with sufficient precision one should be able to get excellent quant on pyrite, pyrrhotite, sulfate and toilite, using the same standard, by using the integrated intensity scan method... without knowing the exact peak position in advance!
Some one should do that and post it here!
You'll need a decent integration time, and I'd bring in the backgrounds a little closer to the peak as we don't need to spend too much time on the tails, but not too close, so as to allow for the expected peak shifting!
Quote from: BenjaminWade on June 05, 2016, 05:12:51 PM
Awesome, thanks again John. I was trying to alter it via wavescan timing, but didn't even think of using the on peak count time to alter it.
I guess one way to look at it is, that although we are really just running a tight wavescan on the peak, because it is for quantitative analysis of unknowns and standards, I decided to use the on-peak time (and the off-peak times as well for the background correction which is subtracted from the integrated intensity to get a net intensity for quantification). Hence why we specify the total integration time rather than the count time per point as in a traditional wavescan.
john
So I ran some integrated intensity scans on pyrite, pyrrhotite and anhydrite and the results are interesting. I ran both with the step/count method which utilizes a variable step size to concentrate more points on the peaks and also ran a straight ROM scan which uses a fixed step size.
Attached below (you must be logged in to see them), are the scans using the step/count method (variable step size). Here are the quant running pyrite against itself:
ELEM: S S S S S Fe Ti SUM
XRAY: (ka) (ka) (ka) (ka) (ka) () ()
235 51.565 51.655 51.492 51.731 51.550 46.550 .058 304.601
236 51.432 51.428 51.512 51.306 51.520 46.550 .058 303.807
AVER: 51.499 51.542 51.502 51.518 51.535 46.550 .058 304.204
SDEV: .094 .160 .014 .301 .021 .000 .000 .561
SERR: .067 .113 .010 .213 .015 .000 .000
%RSD: .18 .31 .03 .58 .04 .00 .00
PUBL: 53.450 53.450 53.450 53.450 53.450 46.550 .058 100.058
%VAR: (-3.65) (-3.57) (-3.64) (-3.61) (-3.58) .00 .00
DIFF: (-1.95) (-1.91) (-1.95) (-1.93) (-1.91) .000 .000
STDS: 730 730 730 730 730 --- ---
Note that the concentrations of sulfur are low, because we measured sulfur on all 5 channels. This results in a non-physical matrix correction. Turning on the "aggregate" mode we now get this for the quant:
ELEM: S S S S S Fe Ti SUM
XRAY: (ka) (ka) (ka) (ka) (ka) () ()
235 53.488 .000 .000 .000 .000 46.550 .058 100.096
236 53.365 .000 .000 .000 .000 46.550 .058 99.973
AVER: 53.427 .000 .000 .000 .000 46.550 .058 100.035
SDEV: .087 .000 .000 .000 .000 .000 .000 .087
SERR: .062 .000 .000 .000 .000 .000 .000
%RSD: .16 .0000 .0000 .0000 .0000 .00 .00
PUBL: 53.450 n.a. n.a. n.a. n.a. 46.550 .058 100.058
%VAR: (-.04) (.00) (.00) (.00) (.00) .00 .00
DIFF: (-.02) --- --- --- --- .000 .000
STDS: 730 0 0 0 0 --- ---
As expected since it is assigned to itself. What about pyrrhotite?
ELEM: S S S S S Fe SUM
XRAY: (ka) (ka) (ka) (ka) (ka) ()
238 39.518 .000 .000 .000 .000 59.808 99.326
239 39.428 .000 .000 .000 .000 59.808 99.236
AVER: 39.473 .000 .000 .000 .000 59.808 99.281
SDEV: .063 .000 .000 .000 .000 .000 .063
SERR: .045 .000 .000 .000 .000 .000
%RSD: .16 .0000 .0000 .0000 .0000 .00
PUBL: 39.580 n.a. n.a. n.a. n.a. 59.808 99.388
%VAR: -.27 .00 .00 .00 .00 .00
DIFF: -.107 --- --- --- --- .000
STDS: 730 0 0 0 0 ---
Nice. And now for anhydrite:
ELEM: S S S S S Ca O Sr SUM
XRAY: (ka) (ka) (ka) (ka) (ka) () () ()
203 23.157 .000 .000 .000 .000 29.380 46.881 .300 99.718
204 23.781 .000 .000 .000 .000 29.380 46.881 .300 100.342
205 23.435 .000 .000 .000 .000 29.380 46.881 .300 99.996
206 23.283 .000 .000 .000 .000 29.380 46.881 .300 99.844
207 23.464 .000 .000 .000 .000 29.380 46.881 .300 100.025
AVER: 23.424 .000 .000 .000 .000 29.380 46.881 .300 99.985
SDEV: .235 .000 .000 .000 .000 .000 .000 .000 .235
SERR: .105 .000 .000 .000 .000 .000 .000 .000
%RSD: 1.00 .0000 .0000 .0000 .0000 .00 .00 .00
PUBL: 23.499 n.a. n.a. n.a. n.a. 29.380 46.881 .300 100.060
%VAR: -.32 .00 .00 .00 .00 .00 .00 .00
DIFF: -.075 --- --- --- --- .000 .000 .000
STDS: 730 0 0 0 0 --- --- ---
The anhydrite scan was run using a shorter count time than the sulfides to avoid sample damage. But it is clear that using the integrated intensity method provides quantitative results when one does not know in advance the emission peak position.
Before someone mentions it, yes there is something funky about my PET crystal on spectro 1. Below are scans from spectro 2 and 4 which look much more normal...
Anyone know what might be the problem with spectro 1?
Hi John
This is interesting. I am keen to give it a go myself at a suitable opportunity. Just for clarification......... The on-peak interference correction procs work in usual way when the integrated intensity technique is used?
As a MAN aficionado, I am wondering whether this technique couldn't be expanded to include rather than off-peak positions, high and low peak limits that could be integrated and used for MAN. Might sound mad, but what do you think? Obviously choice of positions would need to be such that any peak shifts would be grabbed.
Cheers,
Malc.
Quote from: Malcolm Roberts on June 08, 2016, 09:25:42 PM
Hi John
This is interesting. I am keen to give it a go myself at a suitable opportunity. Just for clarification......... The on-peak interference correction procs work in usual way when the integrated intensity technique is used?
As a MAN aficionado, I am wondering whether this technique couldn't be expanded to include rather than off-peak positions, high and low peak limits that could be integrated and used for MAN. Might sound mad, but what do you think? Obviously choice of positions would need to be such that any peak shifts would be grabbed.
Cheers,
Malc.
Hi Malcolm,
Maybe crazy, but it could work, I guess, but the MAN standards would have to be acquired using integrated intensities as well... worth a try I guess.
But yes, the interference corrections should work with integrated intensities also. Frankly I was just pleased that the aggregate mode worked fine for these integrated intensities!
john
Hi John
Another question..... Does the interference correction have to be applied using an equivalent counting technique? By that I mean, if I want to measure element A using the integrated method, and element A has an interference from element B, do I need to acquire element B using the integrated method too or are the on-peak methods fine to go with? My gut-feeling is to use the same approach with both.........
Cheers,
malc.
Quote from: Malcolm Roberts on June 13, 2016, 06:47:10 PM
Hi John
Another question..... Does the interference correction have to be applied using an equivalent counting technique? By that I mean, if I want to measure element A using the integrated method, and element A has an interference from element B, do I need to acquire element B using the integrated method too or are the on-peak methods fine to go with? My gut-feeling is to use the same approach with both.........
Cheers,
malc.
Hi Malcolm,
Great question but I think you'll be fine for the interference correction between integrated and peak intensities. Why do I think so? Because this:
http://smf.probesoftware.com/index.php?topic=482.msg2826#msg2826
Think of it as though one were performing an interference correction between a normal sized WDS analyzing crystal and a large WDS analyzing crystal. As long as the interference standard and the unknown are both measured using the same spectrometer (and element and x-ray), "it all comes out in the wash" as they say!
john
Hi John
Many thanks for doing that test, interesting. The student is yet to be back to reanalyse them but will hopefully get to try out the integrated intensities again soon.
Cheers