I assign my EPMA class a problem; to do a matrix correction by hand. That is week one. Week two is to use CalcZAF. This way they get a flavor of what is in the 'grey box' (not a black box) of the matrix correction.
It occurred to me that it might be a useful instructional exercise if CalcZAF offered an option, wherein ALL (each one) of a series of iterations for determining the various sub-units of the matrix correction could be output, so that (1) they can compare some of their own "by hand" calculations with the 'grey box' results as well as (2) see how much gets changed for each iteration. Would it be possible to have an option to output the sub-steps? Even if dumped into an ascii file which could be viewed.
Quote from: JohnF on November 02, 2016, 02:50:34 PM
I assign my EPMA class a problem; to do a matrix correction by hand. That is week one. Week two is to use CalcZAF. This way they get a flavor of what is in the 'grey box' (not a black box) of the matrix correction.
It occurred to me that it might be a useful instructional exercise if CalcZAF offered an option, wherein ALL (each one) of a series of iterations for determining the various sub-units of the matrix correction could be output, so that (1) they can compare some of their own "by hand" calculations with the 'grey box' results as well as (2) see how much gets changed for each iteration. Would it be possible to have an option to output the sub-steps? Even if dumped into an ascii file which could be viewed.
What a good idea! I will add that tonight.
Hi John,
Ok, I added code to output the iteration results if both DebugMode and VerboseMode flags are true. Here is an example of the output, the text in red is the new iteration output:
Entering ZAFSmp...
Takeoff = 40, Kilovolts = 15
ELEMENT fe ka si ka o ka
UNK WT% .0000 .0000 .0000
UNK CNT 7568.10 1329.40 2519.60
STD WT% 72.0800 46.7400 27.6400
STD CNT 10265.7 5268.20 2498.10
RAWKRAT .737222 .252344 1.00861
STDKFAC .678126 .410094 .194818
FluTyp LinWt FluYld JmpFac MACSmp FluRay MACFlu
Si ka by Fe ka, 1 1.00 .355000 .915063 1.74e+03 1 6.34e+01
O ka by Fe la, 3 4.20 .006300 .946179 3.85e+03 3 4.61e+03
O ka by Si ka, 1 1.00 .050000 .946179 3.85e+03 1 1.74e+03
O ka by Si kb, 2 .050 .050000 .946179 3.85e+03 2 1.53e+03
NORMELEM fe ka si ka o ka
Conc*100 53.9766 14.0563 31.9671
ZAFSmp: Iteration #1
ELEMENT fe ka si ka o ka
ZAFAbs: .9985 1.4398 1.8665
ZAFFlu: 1.0000 .9992 .9945
ZAFZed: 1.0795 .9425 .8750
ZAFCOR: 1.0779 1.3560 1.6241
UNKRAT: .4999 .1035 .1965
UNCONC: .5398 .1406 .3197
FluTyp LinWt FluYld JmpFac MACSmp FluRay MACFlu
Si ka by Fe ka, 1 1.00 .355000 .915063 1.62e+03 1 6.06e+01
O ka by Fe la, 3 4.20 .006300 .946179 3.69e+03 3 5.31e+03
O ka by Si ka, 1 1.00 .050000 .946179 3.69e+03 1 1.62e+03
O ka by Si kb, 2 .050 .050000 .946179 3.69e+03 2 1.42e+03
NORMELEM fe ka si ka o ka
Conc*100 54.7809 13.8219 31.3973
ZAFSmp: Iteration #2
ELEMENT fe ka si ka o ka
ZAFAbs: .9978 1.3995 1.8054
ZAFFlu: 1.0000 .9993 .9956
ZAFZed: 1.0994 .9561 .8900
ZAFCOR: 1.0970 1.3372 1.5997
UNKRAT: .4999 .1035 .1965
UNCONC: .5478 .1382 .3140
FluTyp LinWt FluYld JmpFac MACSmp FluRay MACFlu
Si ka by Fe ka, 1 1.00 .355000 .915063 1.64e+03 1 6.08e+01
O ka by Fe la, 3 4.20 .006300 .946179 3.70e+03 3 5.25e+03
O ka by Si ka, 1 1.00 .050000 .946179 3.70e+03 1 1.64e+03
O ka by Si kb, 2 .050 .050000 .946179 3.70e+03 2 1.43e+03
NORMELEM fe ka si ka o ka
Conc*100 54.7326 13.8542 31.4132
ZAFSmp: Iteration #3
ELEMENT fe ka si ka o ka
ZAFAbs: .9979 1.4036 1.8079
ZAFFlu: 1.0000 .9993 .9955
ZAFZed: 1.0976 .9549 .8886
ZAFCOR: 1.0953 1.3394 1.5994
UNKRAT: .4999 .1035 .1965
UNCONC: .5473 .1385 .3141
FluTyp LinWt FluYld JmpFac MACSmp FluRay MACFlu
Si ka by Fe ka, 1 1.00 .355000 .915063 1.64e+03 1 6.08e+01
O ka by Fe la, 3 4.20 .006300 .946179 3.70e+03 3 5.25e+03
O ka by Si ka, 1 1.00 .050000 .946179 3.70e+03 1 1.64e+03
O ka by Si kb, 2 .050 .050000 .946179 3.70e+03 2 1.43e+03
NORMELEM fe ka si ka o ka
Conc*100 54.7315 13.8508 31.4177
ZAFSmp: Iteration #4
ELEMENT fe ka si ka o ka
ZAFAbs: .9979 1.4033 1.8082
ZAFFlu: 1.0000 .9993 .9955
ZAFZed: 1.0977 .9549 .8887
ZAFCOR: 1.0954 1.3392 1.5998
UNKRAT: .4999 .1035 .1965
UNCONC: .5473 .1385 .3142
Entering ZAFCalZBar...
ELEMENT fe ka si ka o ka
UNK WT% 54.7619 13.8585 31.4352
ZAF correction factors for unknown line 2
ELEMENT fe ka si ka o ka
ZAFAbs: .9979 1.4033 1.8082
ZAFFlu: 1.0000 .9993 .9955
ZAFZed: 1.0977 .9549 .8887
ZAFCOR: 1.0954 1.3392 1.5998
ZAFSTP: 1.1370 .9279 .8337
ZAFBKS: .9655 1.0292 1.0660
STDKFAC .6781 .4101 .1948
UNKKFAC .4999 .1035 .1965
UNKZBAR 18.6827
ZAFITER 4.00
MANITER .00
HAL->O2 .000
ELEMENT fe ka si ka o ka
UNK WT% 54.7619 13.8585 31.4352
ZAF%ERR .0012 .0034 .0046
STDELEM 6 6 6
STDDENS 2.10 2.10 2.10
STDTHIC 200.0 200.0 200.0
STDSINT 311.1 311.1 311.1
SAMPLE: 2, TOA: 40, ITERATIONS: 4, Z-BAR: 18.68271
ELEMENT ABSCOR FLUCOR ZEDCOR ZAFCOR STP-POW BKS-COR F(x)u Ec Eo/Ec MACs uZAF/sZAF
Fe ka .9979 1.0000 1.0977 1.0954 1.1370 .9655 .9867 7.1120 2.1091 60.8022 1.030540
Si ka 1.4033 .9993 .9549 1.3392 .9279 1.0292 .6453 1.8390 8.1566 1635.92 1.174991
O ka 1.8082 .9955 .8887 1.5998 .8337 1.0660 .3876 .5317 28.2114 3698.75 1.127602
ELEMENT K-RAW K-VALUE ELEMWT% OXIDWT% ATOMIC% FORMULA KILOVOL
Fe ka .73722 .49993 54.762 ----- 28.516 .665 15.00
Si ka .25234 .10348 13.859 ----- 14.349 .335 15.00
O ka 1.00861 .19649 31.435 ----- 57.135 1.333 15.00
TOTAL: 100.056 ----- 100.000 2.333