News:

:) To post in-line images, login and click on the Gallery link at the top

Main Menu

SF from inclusion

Started by Ben Buse, February 05, 2025, 06:21:48 AM

Previous topic - Next topic

Ben Buse

Hi

Whilst in GUI can by an inclusion in a host, it seems to be centered on the host

Can you set a distance away from the inclusion within the host to measure the amount of SF from the inclusion on host measurement

Thanks

Ben Buse

#1
It be great to do this by dtsa2 GUI

I'm trying to do this by code using embeded sphere and xtraparameters configurebeam which is defined as

def configureBeam(x, y, z, szNm):
  """configureBeam(x,y,z, szNm)
  Create xtraParams entries to configure the beam for the simulation.
  Input:
  x, y, z - positions of the beam in meters
  szNm    - the beam diameter in nm (converted to m internally)"""
  return { "PosX" : x, "PosY" : y, "PosZ": z, "nmSize": szNm}

however I get the following error

Traceback (most recent call last):
  File "<stdin>", line 8, in <module>
  File "C:/DTSAii/SimpleSimulationScript_withPhiRhoZ_calcite_embedded sphere2.py", line 23
    specSample = mc3.embeddedSphere(sample,0.000000500,matrixsubstrate,0.000000500,det,e0=e0, nTraj=nE, dose=500.0, sf=True, bf=True,xtraParams=xtraP)
    ^
SyntaxError: no viable alternative at input 'specSample'

Any ideas what I'm doing wrong?

The code is
import dtsa2 as dtsa2
import dtsa2.mcSimulate3 as mc3

det = findDetector("SDD") # Replace with your detector's name
nE = 100 # number of electrons simulated
e0 = 15    # kV

sample = epq.Material(epq.Composition(map(dtsa2.element,["Ca","O","C","Mg"],),[0.39,0.48,0.12,0.01],"calcite-Mg"),epq.ToSI.gPerCC(2.84))    # epq.ToSI.gPerCC(2.72) converts 2.65g/cc into SI units 2650 kg/m3, composition is mass fraction
matrixsubstrate = epq.Material(epq.Composition(map(dtsa2.element,["Si","O"],),[0.47,0.53],"quartz"),epq.ToSI.gPerCC(2.65))    # epq.ToSI.gPerCC(2.72) converts 2.65g/cc into SI units 2650 kg/m3, composition is mass fraction
range = dtsa2.electronRange(sample,e0,density=None)

xtraP = {}
#xtraP = {"Characteristic Accumulator":True, "Char Fluor Accumulator":True, "Brem Fluor Accumulator":True}
xtraP.update(mc3.configureXRayAccumulators(mc3.suggestTransitions("CaOCMg",e0),charAccum=True,charFluorAccum=True,bremFluorAccum=True))
#xtraP.update(mc3.configureOutput(DefaultOutput))
xtraP.update(mc3.configurePhiRhoZ(1.5*range))
xtraP.update(mc3.configureEmissionImages(mc3.suggestTransitions("CaOCMg",e0), 1.5*range, size = 512))
xtraP.update(mc3.configureTrajectoryImage(1.5*range, size = 512))
xtraP.update(mc3.configureOutput('C:\DTSAii\Scripts'))    # change to output folder
xtraP.update(mc3.configureBeam(0.000001,0,0,10)
#print xtraP

specSample = mc3.embeddedSphere(sample,0.000000500,matrixsubstrate,0.000000500,det,e0=e0, nTraj=nE, dose=500.0, sf=True, bf=True,xtraParams=xtraP)
specSample.save("%s/%s.msa" % ( 'C:\DTSAii\Scripts', specSample ))        # change to output folder
specSample.display()

Also can the code create the html report?

Ben Buse

#2
Ok something wrong with xtraP

If I try this works but that's without beam configure

xrts=mc3.suggestTransitions("CaOCMg")
xtraParams={}
xtraParams.update(mc3.configureXRayAccumulators(xrts,charAccum=True,charFluorAccum=True,bremFluorAccum=False))
xtraParams.update(mc3.configureEmissionImages(xrts,1.0e-5,512))
xtraParams.update(mc3.configureContinuumImages( ((2.3,2.5), (4.2,4.4 )), 1.0e-5, 512 ))
xtraParams.update(mc3.configurePhiRhoZ(1.0e-5))
xtraParams.update(mc3.configureTrajectoryImage(1.0e-5,512))
#xtraParams.update(mc3.configureVariablePressure(pathLen, gas))
#xtraParams.mc3.configureVRML(nElectrons = 40)
print xtraParams

specSample = mc3.embeddedSphere(sample,0.000000500,matrixsubstrate,0.000000500,det,e0=e0, nTraj=nE, dose=500.0, sf=True, bf=True,xtraParams=xtraParams)
specSample.save("%s/%s.msa" % ( 'C:\DTSAii\Scripts', specSample ))        # change to output folder
specSample.display()


If I include beam configure it fails

xtraParams.update(mc3.configureBeam(0.000001,0,0,10)
And any idea why I have to reboot DTSA-ii for it to run the code again

Nicholas Ritchie

I think you are missing a closing parenthesis.  The interpreter is waiting for the parenthesis when you enter the next command and as a result seems to hang.
"Do what you can, with what you have, where you are"
  - Teddy Roosevelt

Nicholas Ritchie

This works:
import dtsa2 as dtsa2
import dtsa2.mcSimulate3 as mc3

det = findDetector("SDD") # Replace with your detector's name
nE = 100 # number of electrons simulated
e0 = 15    # kV

sample = epq.Material(epq.Composition(map(dtsa2.element,["Ca","O","C","Mg"],),[0.39,0.48,0.12,0.01],"calcite-Mg"),epq.ToSI.gPerCC(2.84))    # epq.ToSI.gPerCC(2.72) converts 2.65g/cc into SI units 2650 kg/m3, composition is mass fraction
matrixsubstrate = epq.Material(epq.Composition(map(dtsa2.element,["Si","O"],),[0.47,0.53],"quartz"),epq.ToSI.gPerCC(2.65))    # epq.ToSI.gPerCC(2.72) converts 2.65g/cc into SI units 2650 kg/m3, composition is mass fraction
range = dtsa2.electronRange(sample,e0,density=None)

xtraP = {}
#xtraP = {"Characteristic Accumulator":True, "Char Fluor Accumulator":True, "Brem Fluor Accumulator":True}
xtraP.update(mc3.configureXRayAccumulators(mc3.suggestTransitions("CaOCMg",e0),charAccum=True,charFluorAccum=True,bremFluorAccum=True))
#xtraP.update(mc3.configureOutput(DefaultOutput))
xtraP.update(mc3.configurePhiRhoZ(1.5*range))
xtraP.update(mc3.configureEmissionImages(mc3.suggestTransitions("CaOCMg",e0), 1.5*range, size = 512))
xtraP.update(mc3.configureTrajectoryImage(1.5*range, size = 512))
xtraP.update(mc3.configureOutput('C:\DTSAii\Scripts'))    # change to output folder
xtraP.update(mc3.configureBeam(0.000001,0,0,10))
print xtraP
specSample = mc3.embeddedSphere(sample,0.000000500,matrixsubstrate,0.000000500,det,e0=e0, nTraj=nE, dose=500.0, sf=True, bf=True,xtraParams=xtraP)
specSample.save("%s/%s.msa" % ( 'C:\DTSAii\Scripts', specSample ))        # change to output folder
specSample.display()
"Do what you can, with what you have, where you are"
  - Teddy Roosevelt

Ben Buse

Thanks for spotting this, obviously I need to use a better editor which will highlight it.

Just wondering whether it's possible to generate the html report result from script

Nicholas Ritchie

Unfortunately, it is not possible to generate the HTML report from a script.
"Do what you can, with what you have, where you are"
  - Teddy Roosevelt

parishcm

Quote from: Nicholas Ritchie on February 19, 2025, 06:44:10 AMUnfortunately, it is not possible to generate the HTML report from a script.

Ha! I logged in today specifically to ask that question. Glad I checked the archive first.

Ben Buse

Any help: what's happening here - if I run the two parts seperately it works in DTSAii, if I run together it works in python but not DTSAii

where code is
createlist=[]
#range as microns
#initial short step
for d in range(0,20,2):
    #store as meters
    print(d)
    createlist.append(float('%s' % float('%.11g' % (d*1e-6))))
#then larger step
#upper limit one extra
for dd in range(20,55,5):
    createlist.append(float('%s' % float('%.11g' % (dd*1e-6))))
    print(dd)

And output in dtsa2 is

Elapse: 0:00:00.0
6> createlist=[]
#range as microns
#initial short step
for d in range(0,20,2):
    #store as meters
    print(d)
    createlist.append(float('%s' % float('%.11g' % (d*1e-6))))
0
2
4
6
8
10
12
14
16
18
Elapse: 0:00:00.0
7> for dd in range(20,55,5):
    createlist.append(float('%s' % float('%.11g' % (dd*1e-6))))
    print(dd)
20
25
30
35
40
45
50
Elapse: 0:00:00.0
8> createlist=[]
#range as microns
#initial short step
for d in range(0,20,2):
    #store as meters
    print(d)
    createlist.append(float('%s' % float('%.11g' % (d*1e-6))))
#then larger step
#upper limit one extra
for dd in range(20,55,5):
    createlist.append(float('%s' % float('%.11g' % (dd*1e-6))))
    print(dd)
  File "<stdin>", line 7
    for dd in range(20,55,5):
    ^
SyntaxError: required (...)+ loop did not match anything at input 'for'
  File "<stdin>", line 1
    createlist.append(float('%s' % float('%.11g' % (dd*1e-6))))
    ^
SyntaxError: no viable alternative at input '    '
  File "<stdin>", line 1
    print(dd)
    ^
SyntaxError: no viable alternative at input '    '
Elapse: 0:00:00.0