Anette von der Handt

Could you add the "absorption edges" checkbox to the KLM markers in the Plot! Wavescans just like you have in the MPB dialog? That would be very useful.
Against the dark, a tall white fountain played.

Anette von der Handt

Two requests around Multi-point backgrounds which I am using a lot lately.

1) Would it be possible to add a "Remove Flags" option (Yes/No) to the "Remove Shared Backgrounds" feature within the "Analyze" menu?
Currently, the function removes shared backgrounds but retains the flags, which can sometimes lead to issues. I would prefer to have the option to choose whether to keep or remove the flags during data processing.

2) Would it be possible to manually select the Multi-Point option as the background type in Element/Cation Properties after searching for Shared Backgrounds? Currently, I can switch from Multi-Point back to Off-Peak, but not the other way around. Sometimes, I want to assess which option works better for a single element, and returning to MPB requires re-searching the shared backgrounds for all elements.

Thank you!
Against the dark, a tall white fountain played.

John Donovan

#692
Quote from: Anette von der Handt on March 30, 2026, 02:15:23 PMCould you add the "absorption edges" checkbox to the KLM markers in the Plot! Wavescans just like you have in the MPB dialog? That would be very useful.

It's already there, just buried one dialog deep:



By the way, this Xray Database dialog also allows one to plot user selected x-ray lines:

John J. Donovan, Pres. 
(541) 343-3400

"Not Absolutely Certain, Yet Reliable"

John Donovan

Quote from: Anette von der Handt on March 30, 2026, 02:29:58 PM1) Would it be possible to add a "Remove Flags" option (Yes/No) to the "Remove Shared Backgrounds" feature within the "Analyze" menu?
Currently, the function removes shared backgrounds but retains the flags, which can sometimes lead to issues. I would prefer to have the option to choose whether to keep or remove the flags during data processing.

I can look into this.


Quote from: Anette von der Handt on March 30, 2026, 02:29:58 PM2) Would it be possible to manually select the Multi-Point option as the background type in Element/Cation Properties after searching for Shared Backgrounds? Currently, I can switch from Multi-Point back to Off-Peak, but not the other way around. Sometimes, I want to assess which option works better for a single element, and returning to MPB requires re-searching the shared backgrounds for all elements.

This is by design because the "Multi-Point" option indicates that MPB data has been acquired, and of course with "shared" MPB samples, the data is loaded from the multiple off-peak elements per spectrometer, not actually acquired.

So you really do need to search again for the off-peak intensities to re-load the shared MPB background intensities and set the MPB flag.
John J. Donovan, Pres. 
(541) 343-3400

"Not Absolutely Certain, Yet Reliable"

dawncruth

#694
Finally (!) playing with sample setups. I'm using the mother of all calibrations (MOAC) approach where I am calibrating all the elements and then building the setup from there. From a glass setup (Si, Al, Ti, Mn, Fe, Mg, Ca, Na, K, Cl, F, etc), I am flagging the Cl, F, K as do not acquire, to make a clinopyroxene setup. In the Sample Setup window in Automate it still lists Cl, F, K as present which is a bit confusing. Is it possible to add a label/flag there that indicates the elements won't be acquired? (see pic for example)

John Donovan

Quote from: dawncruth on April 03, 2026, 05:17:33 PMIs it possible to add a label/flag there that indicates the elements won't be acquired? (see pic for example)

I think this should be relatively easy to do.
John J. Donovan, Pres. 
(541) 343-3400

"Not Absolutely Certain, Yet Reliable"

John Donovan

Quote from: John Donovan on April 03, 2026, 05:50:00 PM
Quote from: dawncruth on April 03, 2026, 05:17:33 PMIs it possible to add a label/flag there that indicates the elements won't be acquired? (see pic for example)

I think this should be relatively easy to do.

Your wish is granted!



Update to the latest Probe for EPMA using the Help menu as usual and you will get this new display feature.  Or download PFE from our Resources page:

https://www.probesoftware.com/resources/
John J. Donovan, Pres. 
(541) 343-3400

"Not Absolutely Certain, Yet Reliable"

Ben Buse

#697
Ability to set beam current at greater than 1000nA, when looking at very low concentration trace elements in stable materials I use the highest beam current which can exceed 1000nA sometimes. Suggest maximum beam current permitted raised to 1.5uA or 2uA.

John Donovan

Quote from: Ben Buse on May 06, 2026, 03:00:21 AMAbility to set beam current at greater than 1000nA, when looking at very low concentration trace elements in stable materials I use the highest beam current which can exceed 1000nA sometimes. Suggest maximum beam current permitted raised to 1.5uA or 2uA.

Your wish is granted!  We modified the max beam current to 2000 nA.

Update as usual from the Help menu.
John J. Donovan, Pres. 
(541) 343-3400

"Not Absolutely Certain, Yet Reliable"

Ben Buse

Thank you, look forward to giving it a go